Beige - Marble
Quarry Location: Apricena, Provincia di Foggia, Puglia
Water Absorption: 0.15 - 0.31 weight-%
Density: 2710 kg/m3
Flexural Strength: 18.5 MPa
Compressive Strength: 218.0 - 242.0 MPa
Recommended Usage: countertops, monuments, mosaic, exterior - interior wall and floor applications, fountains, pool and wall capping, stairs, window sills
Finishing Surface: Polished, Bush Hammered, Tumbled, Brushed, Honed, Split, Machine Cut, Natural Surface, Sandblasted, Acid Washing, Combed, Leathered, Water Jet, Filled, Chiseled, Pickling
Additional Names: Serpeggiante di Apricena Marble, Serpeggiante Apricena Marmo, Serpeggiante Marble, Serpeggiante Apricena Marble
Petrographic definition: limestone
Massa Unit Volume: 2685 kg/m3
Water Absorption: 0.27%
Breaking Load Compression Simple: 218 MPa
Compression breaking load after freezing: 242 MPa
Tensile Strength through indirect Flex: 18.5 MPa
Its coefficient of Abrasion (referred to Granite St. Fedelino): 0.99
Impact resistance: minimum fall height: 25 cm
Linear thermal expansion coefficient of 4.4 x 10-5 0C-1
Knoop microhardness: 1736 MPa
Index unevenness of hardness: 1.16
Source: Universitàdi Pisa - Politecnico di Torino